Voiding under a full copper pour
Several dozen DPAK MOSFETs in parallel, every tab soldered to one continuous copper plane. Thermally that is the right design. At reflow it is the hardest place on the board to keep voiding out of — and the first-article X-ray did not pass the customer's incoming gate.
The solder was fine. The gas had nowhere to go.
The failure was not wetting, and it was not placement. A copper pour that large holds heat evenly, which is exactly why it also traps the volatiles coming off the flux. They expand under the part, the alloy skins over first, and the bubbles stay.
Voids collect directly beneath the die. On a power MOSFET that is the worst possible location: it raises junction temperature, narrows the current margin, and shows up months later as a field failure rather than a line reject.
This is why the customer's gate rejected the first article even though the joints looked perfect from above.

Three adjustments, in the order they matter
None of them is exotic. The point is that they were changed together and then held — a single knob turned on its own just moves the void somewhere else on the board.
Stencil aperture
The aperture went from one continuous opening to a partitioned array over the thermal pad. Less paste per unit area, and deliberate channels for gas to escape sideways instead of pooling under the die.
Trade-off handled: too little paste creates its own problem — poor thermal contact. The window was found by trial, not by guesswork.
Solder paste
Switched to a low-voiding formulation and enforced proper warm-up before the jar is opened. Paste that goes in cold pulls moisture out of the air, and that moisture becomes steam at reflow — the single most common source of voids nobody accounts for.
Reflow profile
Longer soak so the flux volatiles leave before the alloy fully liquidus, a slower ramp through the preheat, and a controlled cool-down. The peak did not go up; the time at temperature was redistributed.
What the X-ray actually measured
Three sample points on the finished assembly, measured with a 6600T at 8.33× magnification. Figures below are taken directly from the inspection report dated 21 September 2026.
| Sample | Pad outline area | Largest single void | Largest void share | Total void area | Total void share | Verdict |
|---|---|---|---|---|---|---|
| 1 | 107,480 | 1,370 | 1.27% | 3,758 | 3.50% | OK |
| 2 | 121,806 | 647 | 0.53% | 5,286 | 4.34% | OK |
| 3 | 122,774 | 677 | 0.55% | 6,239 | 5.08% | OK |
Areas are in square pixels at the inspection magnification; the percentages are what matters. Largest single void 1.27%, total void 3.50–5.08%, all three points pass.
Stable voiding is cheaper than inspected voiding
A process that drifts has to be caught by inspection, and inspection has to be paid for in every quote — extra X-ray sampling, rework capacity, scrap allowance, and the buffer a supplier adds when it cannot predict its own yield.
What an unstable process costs you
- SamplingX-ray on every lot instead of on the first article
- ReworkHot-air rework on a thermal pad is slow and risks the part
- BufferA supplier who is unsure of yield prices the uncertainty in
- Field riskVoids under a die fail late, not on the line
What a held window buys you
- Predictable yieldThe quote reflects the process, not a hedge
- Less inspectionFirst-article plus periodic check, not lot-by-lot
- RepeatabilityBatch two behaves like batch one
- Margin you can design withThermal headroom stays where your engineer put it